Posting this for others to see in case you run into the same thing. I am printing a new, improved version of a case that I designed. I am printing in PETG-CF. Photos 1-3 are where I started, and photos 4-6 are after making adjustments.
I noticed a few residual artifacts from the infill made their way to the surface on this version. When I started printing the lid to the case, which has a much larger flat surface area, I noticed that I was getting a ton of “submerged logs sticking out of the water” and didn’t know why. Turns out the default print speeds were just too high, causing the solid infill to leave spiky residuals behind.
The two main issues were 1, the bridges aren’t bridging properly at the default 25mm/s even with 100-% part cooling fan, and 2, the solid infill and top surface speeds are wayyyy too fast.
For 1, I still need to run some bridge tests, but in the meantime…
For 2, I slowed down the solid infill speed from the default 180mm/s to 60mm/s and the top surface layers down from the…